Moisture Uptake and Dimensional Stability of PC Screws: Test Methods and Criteria
Moisture Uptake and Dimensional Stability of PC Screws: Test Methods and Criteria
Some complaints are hard to reproduce: the customer measures the diameter above the upper limit while the supplier measured it in spec before shipping; the customer says the thread will not start while the supplier installs the same lot without effort. Neither is lying; the samples differ in moisture state. Polycarbonate absorbs water from the environment, swells slightly, and its dimensions, strength and toughness shift accordingly. Most such disputes on PC screw projects are settled by aligning the conditioning state and the measurement sequence.
How moisture uptake happens
Water enters the amorphous regions of PC and occupies space between molecular chains, acting as a plasticiser. The process is reversible and its rate depends on temperature, humidity and wall thickness. Thin parts such as an M3 screw can take up a substantial share of equilibrium moisture within days at 50 percent relative humidity, while thick sections need weeks or more.
Coupling between dimensional change and thread fit
Threads are the most sensitive feature. Crest height is only a few tenths of a millimetre, so even a small percentage change in pitch diameter alters gauge acceptance. Worse, moulding shrinkage is anisotropic, differing along and across the flow direction, and moisture swelling shows a similar directional bias. Different directions therefore change by different amounts, affecting roundness.
Drawings and inspection specifications should state the measurement state explicitly, for example measured after conditioning to equilibrium, or measured dry with acceptance converted from the conditioned basis. Without this clause the two parties will never agree. A common industry practice is for both sides to measure at the approval stage and record the difference as a conversion reference.
Common test methods and their limits
Dimensional stability can also be studied by thermomechanical analysis of the response to temperature change, but for products like plastic screws the engineering interest is behaviour under actual service conditions rather than laboratory curves.
How to condition parts
Conditioning brings products to a known and stable moisture state before inspection and assembly. The usual approach holds parts in a constant temperature and humidity environment for a specified time, with conditions chosen by material and wall thickness and duration confirmed by gravimetric equilibrium. A few days usually suffice for small screws, longer for thicker nuts or washers.
Without a climate chamber, saturated salt solutions in a sealed container provide a stable humidity at very low cost. The essential point is to write the step into the process rather than relying on ambient storage. Seasonal differences are large, and equilibrium moisture in the rainy season differs markedly from winter, so uncontrolled storage guarantees drift between lots.
How strength and toughness change
This creates a selection trade-off: one screw rarely satisfies both crack-free assembly and long-term tightness. The practical answer is to separate the two: control torque and tooling at the assembly end, and absorb relaxation with elastic compensation at the service end. Loading both requirements onto material state usually sacrifices one.
Test conditions for torque and failure strength
Failure torque of PC screws is highly sensitive to loading rate and temperature. Fast loading reads high, high temperature reads low. Test conditions must therefore be fixed and reported, including ambient temperature, loading rate, clamping method and thread engagement depth. Data from different laboratories is comparable only when conditions match.
The effect of engagement depth is often underestimated. Plastic threads distribute stress over a short length, so shallow engagement reduces load-bearing threads and lowers the reading, while excessive engagement hits the hole bottom or stud end and adds parasitic resistance. A stop on the test fixture keeps engagement depth consistent.
Packaging and storage effects
The moisture barrier of packaging determines the condition on arrival. Aluminium foil laminate bags outperform ordinary PE bags considerably, and a desiccant further lowers in-bag humidity. For precision threaded parts, foil bags with desiccant and a sealing date are recommended.
Storage conditions matter equally. Warehouses near external walls or roofs see condensation from day-night temperature swings, and cartons on the floor draw moisture from below. Racking away from walls and off the floor, plus a re-inspection interval for long stock, costs little yet effectively reduces out-of-tolerance on arrival.
Making the acceptance basis work
A workable framework has three parts: a defined inspection state, either conditioned or dry; a defined measurement method with gauges primary and instruments secondary; and a defined dispute route, retesting in a state both parties confirm. Written into the approval document, these three settle most dimensional disputes technically rather than commercially.